<?xml version="1.0" encoding="UTF-8"?><!DOCTYPE article  PUBLIC "-//NLM//DTD Journal Publishing DTD v3.0 20080202//EN" "http://dtd.nlm.nih.gov/publishing/3.0/journalpublishing3.dtd"><article xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink" dtd-version="3.0" xml:lang="en" article-type="research article"><front><journal-meta><journal-id journal-id-type="publisher-id">MSA</journal-id><journal-title-group><journal-title>Materials Sciences and Applications</journal-title></journal-title-group><issn pub-type="epub">2153-117X</issn><publisher><publisher-name>Scientific Research Publishing</publisher-name></publisher></journal-meta><article-meta><article-id pub-id-type="doi">10.4236/msa.2017.86032</article-id><article-id pub-id-type="publisher-id">MSA-76868</article-id><article-categories><subj-group subj-group-type="heading"><subject>Articles</subject></subj-group><subj-group subj-group-type="Discipline-v2"><subject>Chemistry&amp;Materials Science</subject></subj-group></article-categories><title-group><article-title>
 
 
  A Potential Corrosion Inhibitor for Acid Corrosion of Mild Steel
 
</article-title></title-group><contrib-group><contrib contrib-type="author" xlink:type="simple"><name name-style="western"><surname>Osarolube</surname><given-names>Eziaku</given-names></name><xref ref-type="aff" rid="aff1"><sub>1</sub></xref><xref ref-type="corresp" rid="cor1"><sup>*</sup></xref></contrib></contrib-group><aff id="aff1"><label>1</label><addr-line>Department of Physics, University of Port Harcourt, Port Harcourt, Nigeria</addr-line></aff><author-notes><corresp id="cor1">* E-mail:<email>eziaku68@yahoo.com</email></corresp></author-notes><pub-date pub-type="epub"><day>07</day><month>06</month><year>2017</year></pub-date><volume>08</volume><issue>06</issue><fpage>476</fpage><lpage>483</lpage><history><date date-type="received"><day>April</day>	<month>29,</month>	<year>2017</year></date><date date-type="rev-recd"><day>Accepted:</day>	<month>June</month>	<year>11,</year>	</date><date date-type="accepted"><day>June</day>	<month>14,</month>	<year>2017</year></date></history><permissions><copyright-statement>&#169; Copyright  2014 by authors and Scientific Research Publishing Inc. </copyright-statement><copyright-year>2014</copyright-year><license><license-p>This work is licensed under the Creative Commons Attribution International License (CC BY). http://creativecommons.org/licenses/by/4.0/</license-p></license></permissions><abstract><p>
 
 
  1-Phenyl-3-methylpyrazol-5-one (HPMP) was evaluated as corrosion inhibitor for mild steel in hydrochloric, nitric and perchloric acid solutions, using weight loss measurements at room temperature. HPMP was found to retard the corrosion rate of mild steel in hydrochloric and nitric acid solutions, while it aided the corrosion of same metal in perchloric acid solution. Corrosion rate decreased linearly with degree of surface coverage, and higher values of half-life were obtained for the coupons coated with HPMP inhibitor. The thicker the film of the HPMP coating on the metal, the more protection it gave to it, giving rise to the increase in inhibition efficiency.
 
</p></abstract><kwd-group><kwd>Corrosion</kwd><kwd> Mild Steel</kwd><kwd> Film Thickness</kwd><kwd> 1-Phenyl-3-Methylpyrazol-5-One (HPMP)</kwd><kwd> Weight Loss</kwd><kwd> Surface Coverage</kwd></kwd-group></article-meta></front><body><sec id="s1"><title>1. Introduction</title><p>Metals are the pre-eminent important materials used in structural and decorative applications. Most metals and alloys when used in different human activities are susceptible to different mechanisms of corrosion due to their exposure to different corrosive media. In petroleum industries, mild steel is regularly used in the construction of pipe lines. Many corrosion problems arise in these pipelines due to the aggressiveness of the liquids carried by them [<xref ref-type="bibr" rid="scirp.76868-ref1">1</xref>] .</p><p>Corrosion, deterioration or destruction of metals generally, is an unavoidable but controllable process. One of the methods used to reduce the rate of metallic corrosion is the use of inhibitors [<xref ref-type="bibr" rid="scirp.76868-ref2">2</xref>] . Many studies have been carried out to find suitable organic and inorganic compounds to be used as corrosion inhibitors for mild steel in different aqueous solutions, for example, 1H-1,2,4-triazol-l-yl-methyl- 2-(4-chlorophenoxy) acetate, methocarbamol, Potassium Iodide, Pyridoxal and Pyridoxal hydrochlorides, etc. [<xref ref-type="bibr" rid="scirp.76868-ref3">3</xref>] [<xref ref-type="bibr" rid="scirp.76868-ref4">4</xref>] [<xref ref-type="bibr" rid="scirp.76868-ref5">5</xref>] [<xref ref-type="bibr" rid="scirp.76868-ref6">6</xref>] [<xref ref-type="bibr" rid="scirp.76868-ref7">7</xref>] . These compounds were all found to be good Inhibitors of mild steel. The inhibition of metal corrosion by these compounds is attributed to either the adsorption of inhibitor molecule or the formation of a layer of insoluble complex of the metal on the surface which acts as a barrier between the metal surface and the corrosive medium [<xref ref-type="bibr" rid="scirp.76868-ref8">8</xref>] .</p><p>The present study is aimed at investigating the inhibitive properties of 1-phenyl-3-methylpyrazol-5-one on mild steel in different acid solutions such as Hydrochloric acid, Nitric and perchloric acid, using weight loss and coating methods. Parameters such as half-life and film thickness of HPMP on the metal surface will be calculated to determine the inhibition efficiency of the inhibitor.</p></sec><sec id="s2"><title>2. Experimental Method</title><sec id="s2_1"><title>2.1. Material Preparation</title><p>Mild steel sheets were obtained from the Engineering workshop of University of Port Harcourt, Port Harcourt. The optical image of the as-received metal is as shown in <xref ref-type="fig" rid="fig1">Figure 1</xref>. The sheets were mechanically press cut into 5 cm &#215; 5 cm coupons. The two faces had 50 cm<sup>2</sup> total geometric surface area. Each coupon was perforated with a hole at the side to allow the passage of thread for ease of handling. The metal coupons were mechanically cleaned and polished with emery paper of varying surface finish to expose clean shinning surfaces. Thereafter, the coupons were washed in distilled water to remove dirt and rust, degreased in ethanol, dipped in acetone and finally blown dry with a hand drier. The coupons were stored in a desiccator free of moisture prior to their coating with the inhibitor and their use in corrosion studies.</p><p>1-Phenyl-3-methylpyrazol-5-one (HPMP) used as inhibitor was synthesized using the method by Vogel [<xref ref-type="bibr" rid="scirp.76868-ref10">10</xref>] . It is insoluble in water, but soluble in a mixture</p><fig id="fig1"  position="float"><label><xref ref-type="fig" rid="fig1">Figure 1</xref></label><caption><title> Microstructure of mild steel-courtesy Sun et al. [<xref ref-type="bibr" rid="scirp.76868-ref9">9</xref>] </title></caption><graphic mimetype="image"   position="float"  xlink:type="simple"  xlink:href="http://html.scirp.org/file/4-7701949x2.png"/></fig><p>of ethanol and water. The mild steel coupons were coated with HPMP as discussed in the previous works [<xref ref-type="bibr" rid="scirp.76868-ref11">11</xref>] .</p></sec><sec id="s2_2"><title>2.2. Weight Loss Measurements</title><p>Weight loss measurements were carried out as described in previous works [<xref ref-type="bibr" rid="scirp.76868-ref12">12</xref>] [<xref ref-type="bibr" rid="scirp.76868-ref13">13</xref>] . All the chemicals used were of the analytical grade. The sodium hydroxide pellets, hydrochloric acid, nitric acid, perchloric acid, ethanol and acetone, were products of May and Baker Limited, Dagenham, England. Distilled water was used for the preparation of all solutions.</p></sec></sec><sec id="s3"><title>3. Experimental Results and Discussion</title><sec id="s3_1"><title>3.1. Analysis of Weight Loss Measurement Results</title><p>The HPMP inhibitor was coated on the mild steel coupons at room temperature, and exposed to three different acidic environments. Their corresponding weight loss data are presented on <xref ref-type="table" rid="table1">Table 1</xref>. HPMP inhibited the corrosion of mild steel in HCI and HNO<sub>3</sub> environments, as lower values of weight loss were recorded for the coated coupons. However, in the perchloric acid environment, the coated samples had higher values of weight loss than the uncoated samples. This signifies that the inhibitor coating on the coupons dissolved, thereby aiding the corrosion of the metal. This behavior is attributed to the fact that HCIO<sub>4</sub> is one of the strongest acids known. It is a stronger acid than sulfuric and nitric acid. Perchloric acid is dangerously corrosive and readily forms potentially explosive mixtures [<xref ref-type="bibr" rid="scirp.76868-ref14">14</xref>] . It is a powerful oxidizing agent and thus causes fast dissolution of the metals.</p></sec><sec id="s3_2"><title>3.2. Corrosion Kinetics</title><p>To characterize the corrosion reaction, the application of the principles of chemical kinetics to corrosion reaction is being explored. Calculated values of Log (W1-∆W) obtained from the weight loss measurements were plotted against</p><table-wrap id="table1" ><label><xref ref-type="table" rid="table1">Table 1</xref></label><caption><title> Weight loss (g) of coated and uncoated Mild Steel coupons in various acid solutions</title></caption><table><tbody><thead><tr><th align="center" valign="middle"  rowspan="2"  >Time (Days)</th><th align="center" valign="middle"  colspan="6"  >Weight loss (g)</th></tr></thead><tr><td align="center" valign="middle"  colspan="2"  >HCI</td><td align="center" valign="middle"  colspan="2"  >HNO<sub>3</sub></td><td align="center" valign="middle"  colspan="2"  >HCIO<sub>4</sub></td></tr><tr><td align="center" valign="middle" ></td><td align="center" valign="middle" >Uncoated coupon</td><td align="center" valign="middle" >Coated coupon</td><td align="center" valign="middle" >Uncoated coupon</td><td align="center" valign="middle" >Coated coupon</td><td align="center" valign="middle" >Uncoated coupon</td><td align="center" valign="middle" >Coated coupon</td></tr><tr><td align="center" valign="middle" >1</td><td align="center" valign="middle" >0.3490</td><td align="center" valign="middle" >0.1346</td><td align="center" valign="middle" >2.4677</td><td align="center" valign="middle" >1.7040</td><td align="center" valign="middle" >0.2975</td><td align="center" valign="middle" >0.3067</td></tr><tr><td align="center" valign="middle" >2</td><td align="center" valign="middle" >0.4573</td><td align="center" valign="middle" >0.2091</td><td align="center" valign="middle" >2.5144</td><td align="center" valign="middle" >1.7855</td><td align="center" valign="middle" >0.4853</td><td align="center" valign="middle" >0.5600</td></tr><tr><td align="center" valign="middle" >3</td><td align="center" valign="middle" >0.6057</td><td align="center" valign="middle" >0.2841</td><td align="center" valign="middle" >2.7345</td><td align="center" valign="middle" >2.0199</td><td align="center" valign="middle" >0.6836</td><td align="center" valign="middle" >0.7929</td></tr><tr><td align="center" valign="middle" >4</td><td align="center" valign="middle" >0.8257</td><td align="center" valign="middle" >0.4256</td><td align="center" valign="middle" >2.9570</td><td align="center" valign="middle" >2.2336</td><td align="center" valign="middle" >0.8984</td><td align="center" valign="middle" >1.0541</td></tr><tr><td align="center" valign="middle" >5</td><td align="center" valign="middle" >1.0074</td><td align="center" valign="middle" >0.5360</td><td align="center" valign="middle" >3.0669</td><td align="center" valign="middle" >2.4968</td><td align="center" valign="middle" >1.0916</td><td align="center" valign="middle" >1.4532</td></tr><tr><td align="center" valign="middle" >6</td><td align="center" valign="middle" >1.1764</td><td align="center" valign="middle" >0.6340</td><td align="center" valign="middle" >3.1332</td><td align="center" valign="middle" >2.7459</td><td align="center" valign="middle" >1.2454</td><td align="center" valign="middle" >1.7359</td></tr><tr><td align="center" valign="middle" >7</td><td align="center" valign="middle" >1.2813</td><td align="center" valign="middle" >0.7888</td><td align="center" valign="middle" >3.1890</td><td align="center" valign="middle" >2.9865</td><td align="center" valign="middle" >1.3822</td><td align="center" valign="middle" >2.0380</td></tr></tbody></table></table-wrap><p>time as shown in <xref ref-type="fig" rid="fig2">Figure 2</xref>. The straight lines obtained from the plots in <xref ref-type="fig" rid="fig1">Figure 1</xref> with or without inhibitor coating confirm a first order reaction kinetics with respect to mild steel in the various acidic medium. A similar result was reported earlier for the corrosion of mild steel in HCI solution [<xref ref-type="bibr" rid="scirp.76868-ref15">15</xref>] .</p><p>The first rate equation was used to evaluate the rate constant since the dissolution of mild steel for both the uncoated and coated samples in the acid solutions obey the first order rate equation. The rate constants (k) at room temperature were used to calculate the half-life (t<sub>1/2</sub>) of the system by making use of the first order reaction equation [<xref ref-type="bibr" rid="scirp.76868-ref16">16</xref>] .</p><disp-formula id="scirp.76868-formula299"><label>(1)</label><graphic position="anchor" xlink:href="http://html.scirp.org/file/4-7701949x3.png"  xlink:type="simple"/></disp-formula><p>where k is the rate constant calculated using Equation (1).</p><disp-formula id="scirp.76868-formula300"><label>(2)</label><graphic position="anchor" xlink:href="http://html.scirp.org/file/4-7701949x4.png"  xlink:type="simple"/></disp-formula><p>where W<sub>i</sub> is the initial weight of the sample, W<sub>f</sub> is the final weight of the sample and t is the immersion time (days). The calculated values of rate constants (k)</p><fig id="fig2"  position="float"><label><xref ref-type="fig" rid="fig2">Figure 2</xref></label><caption><title> Variation of log (W<sub>1</sub>-ΔW) with time (days) for uncoated and coated mild steel in 0.5 m HCl, HNO<sub>3</sub> and HClO<sub>4</sub> solutions</title></caption><graphic mimetype="image"   position="float"  xlink:type="simple"  xlink:href="http://html.scirp.org/file/4-7701949x5.png"/></fig><p>and half-life (t<sub>1/2</sub>) obtained from Equation (1) are presented on <xref ref-type="table" rid="table2">Table 2</xref>. The results further confirm the inhibition of the metal by HPMP as higher values of half-life were obtained for the coated samples. For instance, for the uncoated mild steel coupon in HCI solution, it will take about 56.3 days for half of the coupon to decay (deteriorate) while for the coupon coated with HPMP, It will take about 113.3 days for half of the coupon to decay or corrode. This is a proof that HPMP is an effective corrosion inhibitor for mild steel. HPMP must have retarded corrosion by adsorption to form a thin invisible film only a few micrometers thick.</p></sec><sec id="s3_3"><title>3.3. Variation of Corrosion Rate with Surface Coverage</title><p>The plot of the results of corrosion rate evaluated by Equation (3) is as shown on <xref ref-type="fig" rid="fig3">Figure 3</xref>.</p><fig id="fig3"  position="float"><label><xref ref-type="fig" rid="fig3">Figure 3</xref></label><caption><title> Variation of corrosion rates (mpy) with surface coverage (Ɵ) of HPMP inhibitor on mild steel in 0.5 m acid solution</title></caption><graphic mimetype="image"   position="float"  xlink:type="simple"  xlink:href="http://html.scirp.org/file/4-7701949x6.png"/></fig><table-wrap id="table2" ><label><xref ref-type="table" rid="table2">Table 2</xref></label><caption><title> Kinetic parameters for uncoated and coated mild steel in acid solutions</title></caption><table><tbody><thead><tr><th align="center" valign="middle" >Nature of coupon</th><th align="center" valign="middle" >Acid</th><th align="center" valign="middle" >Rate Constant K (day<sup>−1</sup>)</th><th align="center" valign="middle" >Half-life, t<sub>1/2</sub> (days)</th></tr></thead><tr><td align="center" valign="middle" >Uncoated</td><td align="center" valign="middle" >0.05M HCl</td><td align="center" valign="middle" >0.0123</td><td align="center" valign="middle" >56.3</td></tr><tr><td align="center" valign="middle" >Coated</td><td align="center" valign="middle" >0.05M HCl</td><td align="center" valign="middle" >0.0052</td><td align="center" valign="middle" >113.3</td></tr><tr><td align="center" valign="middle" >Uncoated</td><td align="center" valign="middle" >0.05M HNO<sub>3</sub></td><td align="center" valign="middle" >0.0323</td><td align="center" valign="middle" >21.5</td></tr><tr><td align="center" valign="middle" >Coated</td><td align="center" valign="middle" >0.05M HNO<sub>3</sub></td><td align="center" valign="middle" >0.0169</td><td align="center" valign="middle" >41.0</td></tr><tr><td align="center" valign="middle" >Uncoated</td><td align="center" valign="middle" >0.05M HClO<sub>4</sub></td><td align="center" valign="middle" >0.0133</td><td align="center" valign="middle" >52.1</td></tr><tr><td align="center" valign="middle" >Coated</td><td align="center" valign="middle" >0.05M HClO<sub>4</sub></td><td align="center" valign="middle" >0.0205</td><td align="center" valign="middle" >43.6</td></tr></tbody></table></table-wrap><disp-formula id="scirp.76868-formula301"><label>(3)</label><graphic position="anchor" xlink:href="http://html.scirp.org/file/4-7701949x7.png"  xlink:type="simple"/></disp-formula><p>where w = weight loss (g) D = density of specimen (g/cm<sup>3</sup>) A = area of specimen (cm<sup>2</sup>) and T is exposure time (hours).</p><p>It is seen from the plot that corrosion rate decreases linearly with the degree of surface coverage for the metal studied. The straight lines confirm that the inhibition is due to the adsorption of HPMP on the metal surface.</p></sec><sec id="s3_4"><title>3.4. Film Thickness (μm) and Inhibition Efficiency (%)</title><p>Variation of film thickness with inhibition efficiency is presented on <xref ref-type="table" rid="table3">Table 3</xref>. The result reveal that the thicker the film of the coating, the more protection it gives to the metal, giving rise to the increase in inhibition efficiency. The negative values of inhibition efficiency obtained for the metal in HClO<sub>4</sub> environment is a further proof that there was no inhibition of the metal in perchloric acid environment. A film thickness of 13.904 μm was obtained for mild steel, which yielded inhibition efficiency of 61.43%. The film forms a blanket over the surface of the metal, blocking the reaction sites (surface defects), thereby protecting the metal from direct attack of the acid.</p><p>The results of Inhibition Efficiency as shown on <xref ref-type="table" rid="table3">Table 3</xref> are evaluated using Equation (4).</p><disp-formula id="scirp.76868-formula302"><label>(4)</label><graphic position="anchor" xlink:href="http://html.scirp.org/file/4-7701949x8.png"  xlink:type="simple"/></disp-formula><p>where W<sub>1</sub> is weight loss of coated sample with inhibitor, and W<sub>2</sub> is weight loss of uncoated sample. <xref ref-type="table" rid="table3">Table 3</xref> reveals that inhibition efficiency decreases with time in the various acidic solutions. The negative values of inhibition efficiency obtained for mild steel signify that there was no inhibition of the metal in HCIO<sub>4</sub> solution. The results also show that the thicker the film of the coating, the more protection it gives to the metals, giving rise to inhibition efficiency. The inhibition of the corrosion process by HPMP can be attributed to adsorption of its molecules at the metal-acid solution interface. This is usually observed by the decrease in corrosion loss as measured by weight loss.</p></sec></sec><sec id="s4"><title>4. Conclusions</title><p>From the present study, it is concluded that HPMP is a potential inhibitor for</p><table-wrap id="table3" ><label><xref ref-type="table" rid="table3">Table 3</xref></label><caption><title> Film thickness (μm) and inhibition efficiency (%) in 0.5 m acid concentration</title></caption><table><tbody><thead><tr><th align="center" valign="middle"  rowspan="2"  >Time (days)</th><th align="center" valign="middle"  colspan="3"  >Film Thickness (μm)</th><th align="center" valign="middle"  colspan="3"  >Inhibition Efficiency (%)</th></tr></thead><tr><td align="center" valign="middle" >HCl</td><td align="center" valign="middle" >HNO<sub>3</sub></td><td align="center" valign="middle" >HClO<sub>4</sub></td><td align="center" valign="middle" >HCl</td><td align="center" valign="middle" >HNO<sub>3</sub></td><td align="center" valign="middle" >HClO<sub>4</sub></td></tr><tr><td align="center" valign="middle" >1</td><td align="center" valign="middle" >13.904</td><td align="center" valign="middle" >12.746</td><td align="center" valign="middle" >13.209</td><td align="center" valign="middle" >61.43</td><td align="center" valign="middle" >30.95</td><td align="center" valign="middle" >−3.09</td></tr><tr><td align="center" valign="middle" >4</td><td align="center" valign="middle" >7.879</td><td align="center" valign="middle" >9.965</td><td align="center" valign="middle" >11.355</td><td align="center" valign="middle" >48.51</td><td align="center" valign="middle" >24.46</td><td align="center" valign="middle" >−17.34</td></tr><tr><td align="center" valign="middle" >7</td><td align="center" valign="middle" >6.025</td><td align="center" valign="middle" >7.647</td><td align="center" valign="middle" >6.025</td><td align="center" valign="middle" >38.44</td><td align="center" valign="middle" >6.35</td><td align="center" valign="middle" >−47.45</td></tr></tbody></table></table-wrap><p>mild steel corrosion in HCI and HNO<sub>3</sub> solutions. All parameters evaluated showed that there was no inhibition in HCIO<sub>4</sub>, as negative values were obtained. Higher values of half-life were obtained for the coated samples, which is a proof that HPMP inhibited the mild steel samples.</p><p>Also the thicker the film of the coating, the more protection it gives to the metals, giving rise to higher inhibition efficiency. The corrosion inhibition by HPMP can be attributed to the adsorption of its molecules at the metal surface.</p></sec><sec id="s5"><title>Acknowledgements</title><p>I am grateful to Professor Israel Owate for his encouragement in this work and also the chemistry laboratory of the University for allowing me have access to their facilities.</p></sec><sec id="s6"><title>Cite this paper</title><p>Eziaku, O. (2017) A Potential Corrosion Inhibitor for Acid Corrosion of Mild Steel. Materials Sciences and Applications, 8, 476-483. https://doi.org/10.4236/msa.2017.86032</p></sec></body><back><ref-list><title>References</title><ref id="scirp.76868-ref1"><label>1</label><mixed-citation publication-type="other" xlink:type="simple">Al-Otaibi, M.S., Al-Mayouf, A.M., Khan, M., Mousa, A.A., Al-Mazroa, S.A. and Alkhathlan, H.Z. (2014) Corrosion Inhibitory Action of Some Plant Extracts on the Corrosion of Mild Steel in Acidic Media. Arabian Journal of Chemistry, 7, 340-346. https://doi.org/10.1016/j.arabjc.2012.01.015</mixed-citation></ref><ref id="scirp.76868-ref2"><label>2</label><mixed-citation publication-type="other" xlink:type="simple">Singh, A., Ahamad, I., Singh, V.K. and Quraishi, M.A. (2011) Inhibition Effect of Environmentally Benign Karanj (Pongamia pinnata) Seed Extract on Corrosion of Mild Steel in Hydrochloric Acid Solution. Journal of Solid State Electrochemistry, 15, 1087-1097. https://doi.org/10.1007/s10008-010-1172-z</mixed-citation></ref><ref id="scirp.76868-ref3"><label>3</label><mixed-citation publication-type="other" xlink:type="simple">Tao, Z., Zhang, S., Li, W. and Hou, B. (2011) Adsorption and Inhibitory Mechanism of 1H-1,2,4-Triazol-l-yl-methyl-2-(4-chlorophenoxy) Acetate on Corrosion of Mild Steel in Acidic Solution. Industrial &amp; Engineering Chemistry Research, 50, 6082-6088. https://doi.org/10.1021/ie101793b</mixed-citation></ref><ref id="scirp.76868-ref4"><label>4</label><mixed-citation publication-type="other" xlink:type="simple">Zerga, B., Attayibat, A., Sfaira, M., Taleb, M., Hammouti, B., Ebn Touhami, M., Radi, S. and Rais, Z. (2010) Effect of Some Tripodal Bipyrazolic Compounds on C38 Steel Corrosion in Hydrochloric Acid Solution. Journal of Applied Electrochemistry, 40, 1575. https://doi.org/10.1007/s10800-010-0164-0</mixed-citation></ref><ref id="scirp.76868-ref5"><label>5</label><mixed-citation publication-type="other" xlink:type="simple">Attar, T., Larabi, L. and Harek, Y. (2014) The Inhibition Effect of Potassium Iodide on the Corrosion of Pure Iron in Sulphuric Acid. Advances in Chemistry, 2014, Article ID: 827514, 5 pages.</mixed-citation></ref><ref id="scirp.76868-ref6"><label>6</label><mixed-citation publication-type="other" xlink:type="simple">Gopi, D., Sherif, El-S.M., Manivannan, V., Rajeswari, D., Surendiran, M. and Kavitha, L. (2014) Corrosion and Corrosion Inhibition of Mild Steel in Groundwater at Different Temperatures by Newly Synthesized Benzotriazole and Phosphono Derivatives. Industrial and Engineering Chemistry Research, 53, 4286-4294. https://doi.org/10.1021/ie4039357</mixed-citation></ref><ref id="scirp.76868-ref7"><label>7</label><mixed-citation publication-type="other" xlink:type="simple">Ebenso, E.E., Eddy, N.O. and Odongenyi, A.O. (2009) Inhibition of the Corrosion of Mild Steel by Methocarbamol. Portugaliae Electrochimica Acta, 27, 13-22. https://doi.org/10.4152/pea.200901013</mixed-citation></ref><ref id="scirp.76868-ref8"><label>8</label><mixed-citation publication-type="other" xlink:type="simple">Okafor, P.C., Liu, C.B., Liu, X., Zheng, Y.G., Wang, F. and Liu, C.Y. (2010) Corrosion Inhibition and Adsorption Behavior of Imidazoline Salt on N80 Carbon Steel in CO2-Saturated Solutions and Its Synergism with Thiourea. Journal of Solid State Electrochemistry, 14, 1367-1376. https://doi.org/10.1007/s10008-009-0963-6</mixed-citation></ref><ref id="scirp.76868-ref9"><label>9</label><mixed-citation publication-type="other" xlink:type="simple">Sun, Y.F., Fujii, H., Takaki, N. and Okitsu, Y. (2012) Microstructure and Mechanical Properties of Mild Steel Joints Prepared by a Flat Friction Stir Spot Welding Technique. Materials and Design, 37, 384-392. https://doi.org/10.1016/j.matdes.2012.01.027</mixed-citation></ref><ref id="scirp.76868-ref10"><label>10</label><mixed-citation publication-type="other" xlink:type="simple">Vogel, A.I. (2002) Text Book of Practical Organic Chemistry. 4th Edition, Longman Ltd., London, 882-889.</mixed-citation></ref><ref id="scirp.76868-ref11"><label>11</label><mixed-citation publication-type="other" xlink:type="simple">Eziaku, O. and James, A.O. (2014) Corrosion Inhibition of Mild Steel in Hydrochloric Acid by African Black Velvet Tamarind. Journal of Emerging Trend in Engineering and Applied Sciences, 5, 51-55.</mixed-citation></ref><ref id="scirp.76868-ref12"><label>12</label><mixed-citation publication-type="journal" xlink:type="simple"><name name-style="western"><surname>Eziaku</surname><given-names> O. </given-names></name>,<etal>et al</etal>. (<year>2014</year>)<article-title>Effect of an Organic Inhibitor on the Electrical Properties of High Carbon Steel in Simulated Acid Environment</article-title><source> Journal of Materials Science and Chemical Engineering</source><volume> 2</volume>,<fpage> 28</fpage>-<lpage>33</lpage>.<pub-id pub-id-type="doi"></pub-id></mixed-citation></ref><ref id="scirp.76868-ref13"><label>13</label><mixed-citation publication-type="other" xlink:type="simple">Eziaku, O., Owate, I.O. and Oforka, N.C. (2008) Corrosion Behaviour of Mild and High Carbon Steels in Various Acidic Media. Scientific Research and Essay, 3, 224-228. http://www.academicjournals.org/SRE</mixed-citation></ref><ref id="scirp.76868-ref14"><label>14</label><mixed-citation publication-type="other" xlink:type="simple">Mendiratta, S.K., Dotson, D.L. and Brooker, R.T. (2005) Perchloric Acid and Perchlorates. Kirk-Othmer Encyclopedia of Chemical Technology.</mixed-citation></ref><ref id="scirp.76868-ref15"><label>15</label><mixed-citation publication-type="other" xlink:type="simple">James, A.O., Oforka, N.C., Abiola, O.K. and Ita, B.I. (2007) A Study on the Inhibition of Mild Steel Corrosion in Hydrochloric Acid by Pyridoxol Hydrochloride. Electica Quimica, 32, 31-36. https://doi.org/10.1590/s0100-46702007000300005</mixed-citation></ref><ref id="scirp.76868-ref16"><label>16</label><mixed-citation publication-type="other" xlink:type="simple">Atkins, P.W. (1980) Chemisorbed and Physisorbed Species: A Textbook of Physical Chemistry. University Press, Oxford, 936-938.</mixed-citation></ref></ref-list></back></article>